Cross-reference table

DD11 equivalents by system
GradeSystemMatchWhy / differences
HR1BS (superseded British)IdenticalBS 1449-1 HR1 (commercial hot-rolled).
IS 1079 DIS (India)IdenticalIS 1079 grade D (drawing) / O (ordinary); D is the DD11 match.
SPHCJIS (Japan)IdenticalJIS G3131 SPHC: C ≤ 0.15, Mn ≤ 0.60, Rm ≥ 270 MPa, A ≥ 27–31 % by thickness. Commercial hot-rolled forming sheet — SPHD ≈ DD12, SPHE ≈ DD13.
CS Type B (A1011)ASTM / ASMENearASTM A1011 Commercial Steel Type B hot-rolled: C ≤ 0.02–0.15, Mn ≤ 0.60, no guaranteed mechanicals. DS (Drawing Steel) Type B corresponds to DD12/DD13.
DD12EN (European)NearDrawing quality with tighter chemistry and higher elongation.
Q195 / SPHCGB/T (China)NearGB/T 5213 hot-rolled uses DD11-type names in newer editions; older specs use Q195 (yield ≥ 195 MPa) or 08Al.
08kp / 08ps hot-rolledGOST (Russia/CIS)NearGOST 16523 group KhP (cold-forming quality) on 08kp/08ps base.
St37-2DIN (superseded German)FunctionalHot-rolled forming sheet often bought 'as St37' in Turkey/Middle East — but it has no guaranteed minimum yield.
DD13EN (European)FunctionalDeep-drawing quality (A ≥ 28–33 %) for demanding pressings.
S235JREN (European)FunctionalStructural steel of similar chemistry with guaranteed 235 MPa yield and impact; DD11 has no minimum yield guarantee for structural design.

Identical = same composition and mechanical limits within rounding. Near = one limit differs (e.g. carbon max or impact temperature). Functional = interchangeable for most uses after an engineering check.

How the matches are graded

Identical means the chemical composition windows overlap so that material certified to one specification meets the other without deviation, and the mechanical minimums are the same or the other is inside them — mills usually dual-certify. Near means one limit differs (a carbon maximum, an impact temperature, a strength minimum or a delivery condition) and a substitution needs a one-line engineering check. Functional means the grades serve the same purpose but are not the same steel — a designer can often use one for the other, but only after re-checking the design.

DD11 in BS (superseded British)

  • HR1Identical BS 1449-1 HR1 (commercial hot-rolled).

DD11 in IS (India)

  • IS 1079 D — Identical IS 1079 grade D (drawing) / O (ordinary); D is the DD11 match.

DD11 in JIS (Japan)

  • SPHC — Identical JIS G3131 SPHC: C ≤ 0.15, Mn ≤ 0.60, Rm ≥ 270 MPa, A ≥ 27–31 % by thickness. Commercial hot-rolled forming sheet — SPHD ≈ DD12, SPHE ≈ DD13.

DD11 in ASTM / ASME

  • CS Type B (A1011) — Near ASTM A1011 Commercial Steel Type B hot-rolled: C ≤ 0.02–0.15, Mn ≤ 0.60, no guaranteed mechanicals. DS (Drawing Steel) Type B corresponds to DD12/DD13.

DD11 in EN (European)

  • DD12 — Near Drawing quality with tighter chemistry and higher elongation.
  • DD13 — Functional Deep-drawing quality (A ≥ 28–33 %) for demanding pressings.
  • S235JRFunctional Structural steel of similar chemistry with guaranteed 235 MPa yield and impact; DD11 has no minimum yield guarantee for structural design.

DD11 in GB/T (China)

  • Q195 / SPHC — Near GB/T 5213 hot-rolled uses DD11-type names in newer editions; older specs use Q195 (yield ≥ 195 MPa) or 08Al.

DD11 in GOST (Russia/CIS)

  • 08kp / 08ps hot-rolled — Near GOST 16523 group KhP (cold-forming quality) on 08kp/08ps base.

DD11 in DIN (superseded German)

  • St37-2Functional Hot-rolled forming sheet often bought 'as St37' in Turkey/Middle East — but it has no guaranteed minimum yield.

Superseded names for DD11

  • StW22 — DIN 1614-1 (withdrawn): Still the common German/Turkish shop name; StW23 = DD12, StW24 = DD13.
  • FeP11 — EN 10111:1991: Renamed DD11 in 1998.
  • HR1 / HR2 — BS 1449-1: HR1 is the nearer match.
  • 1C — NF A 36-301

Key data for DD11

Yield170–360 MPa t < 2 mm (transverse)
Tensile≤ 440 MPa
Carbon≤ 0.12 %
StandardEN 10111

Full composition, mechanical properties by thickness, heat treatment and applications for DD11 →